DH40 Shipbuilding Steel Chemical Composition:
Grade
| C max | Si max | Mn | P max | S max | Als min | Ti max | Cu max | Cr max | Ni max | Mo max | Nb | V |
DH40 | 0.18 | 0.50 | 0.90-1.60 | 0.035 | 0.035 | 0.015 | 0.02 | 0.35 | 0.20 | 0.40 | 0.08 | 0.02-0.05 | 0.05-0.10 |
Note: Generally speaking CE will be ≤ 0.40%. If the delivery condition is TMPC, the CE will be : ≤ 0.40% (thickness ≤ 50mm). Ceq% =(C+Mn)/6+(Cr+Mo+V)/5+(Ni+Cu)/15.
9. DH40 steel plate Mechanical Property
Grade
| Rm (MPa) | Re(MPa) min | A% min | Akv/J min |
DH40 | 510-660 | 390 | 20 | E.T °C | Thickness (mm) |
-20 | ≤ 50 | >50-70 | >70-100 |
L | C | L | C | L | C |
41 | 27 | - |
Note: In the list , Rm: .tensile strength,Re: Yield strength,A%: elongation, E.T: experimental temperature,L: lengthways, C: crosswise.
10. DH40 steel plate Condition Of Delivery
Grade
| Fine grains elements | category | The thickness of steel |
≤ 12 | >12.5-20 | >20-25 | >25-35 | >35-50 | >50-100 |
DH40 | any | Plate/ sheet | A(50) | N(50),CR(50),TM(50) | - |
A. Delivery Condition: As Rolled(AR), Controled Rolling(CR),Thermal Mechanical Control Process(TMCP),Normalizing(N),Tempering(T), Annealing(A), Quenching(Q), Quenching & Tempering(QT).
B. The Ultrasonic inspection can be done according to ASTM A435, ASTM A577, ASTM A578, EN10160, SEL072, NFA 04-305, BS5996 standard.
C. Additional Service: Heat treatment, Charpy V tes, Pre treatment,Cutting,Galvanization.
D. Classification Society like ABS , BV , DNV , GL, KR, LR, NK, RINA.